SDS Volume (4115)
Volume 70. Solubility of Gases in Glassy Polymers, p None
Original Measurements
Variables:
Room Temp:
298
$\pu{K}$
Pressure:
0 - 100
$\pu{kPa}$
Prepared by:
Method/Apparatus/Procedure:
Sorption was studied using a McBain balance with quartz spring. The procedure has been described in [1].
Source and Purity of Materials:
- $\ce{SO2}$: traces of air were removed from the gas prior to use.
PVTMS films: recast after dissolving gas separation PVTMS membrane (NPO Plastmassy) is methylbenzene.
Estimated Errors:
Ambient temperature: No information given.
References
Components:
- Sulfur dioxide, $\ce{ SO2 }$; [7446-09-5] NIST WebBook
- Poly(vinyltrimethyl silane) (PVTMS), $\ce{ (C5H12Si)n }$; [25036-32-2] NIST WebBook
Experimental Data
Dual mode sorption parameters fo SO2 in PVTMS at 298 K
| kD (mol(g)/cm3 Pa-1) | $C_{1}$ (mol/L) | $b$ ($\pu{kPa-1}$) |
|---|---|---|
| 2.0109 | 0.45 | 0.01 |