Components:

(1) Carbon dioxide, CO2; [124-38-9] NIST WebBook
(2) Polystyrene, (C8H8)n; [9003-53-6] NIST WebBook
(3) Poly(vinylmethyl ether), (C3H6O)n; [9003-09-2] NIST WebBook

Original Measurements

Hachisuka, H.; Sato, H.; Tsujita, Y.; Takizawa, A.; Kinoshita, T.; Polym. J. 21, 417-424 (1989).

Variables:

Ambient temperature: 298 K
Pressure: 0 - 1.33 MPa

Prepared by:

Yu.P. Yampol'skii

Method/Apparatus/Procedure:

Sorption measurement was carried out using electromicrobalance Cahn 2000. The correction for buoyancy was introduced.

Source and Purity of Materials:
  1. Type                             PS,%          PVME,%       Tg , K
    Single phase                75                   25                 315.0
    same                             50                  50                 262.9
    same                             20                  80                 248.6
    Phase separated         83                   17                 321.2
    (75/25)                          21                  79                 249.2
    Phase separated         73                   27                 301.2
    (50/50)                          31                   69                 253.2
    Phase separated         74                   26                 308.6
    (20/80)                          19                   81                 248.0

    CO2 purity >99.99%.

Experimental Values:
Dual mode sorption parameters for CO2 in PS/PVME blends
H (cm3(STP)/cm3 cmHg-1) C'H (cm3/cm3) b (cm Hg) Comptot Phase (s)
1.12 x 10-2 4.1 2.36 x 10-3 100/0 Polystyrene
1.41 x 10-2 1.5 1.45 x 10-3 75/25 Single phase blend
2.01 x 10-2 - - 50/50 Single phase blend
2.62 x 10-2 - - 20/80 Single phase blend
1.49 x 10-2 2.4 2.76 x 10-3 75/25 Phase separated blend
2.05 x 10-2 4 x 10-1 4.73 x 10-3 50/50 Phase separated blend
2.93 x 10-2 1.1 3.95 x 10-3 20/80 Phase separated blend
4.00 x 10-2 - - 0/100