SDS Volume (4034)

Volume 70. Solubility of Gases in Glassy Polymers, p None

Original Measurements

Barbari, T. A.; Koros, W. J.; Paul, D. R.; J. Polym. Sci. B: Polym. Phys. 26, 729-744 (1988).

Variables:

Room Temp: 308 $\pu{K}$
Pressure: 0 - 2.3 $\pu{MPa}$

Prepared by:

A.K. Bokarev

Method/Apparatus/Procedure:

The sorption apparatus and procedures used in the present sorption experiments are the same as described earlier [1].

Source and Purity of Materials:
  1. Gas: purity > 99.99% (chromatographic quality). PHI (Ultem): General Electric Co., $\rho = \pu{1.28 g mL-1}$, $T_{\rm{g}}$ = 488 K.
Estimated Errors:

Ambient temperature: No information given.

References

1 Koros, W. J.; Paul, D. R.; Rocha, A. A.; J. Polym. Sci., Polym. Phys. Ed., 1976, 14, 687.

Components:
  1. Nitrogen (Molecule), $\ce{ N2 }$; [7727-37-9] NIST WebBook
  2. Carbon dioxide, $\ce{ CO2 }$; [124-38-9] NIST WebBook
  3. Methane, $\ce{ CH4 }$; [74-82-8] NIST WebBook
  4. Polyetherimide (PEI), [61128-24-3] NIST WebBook
Experimental Data
Table 1. Dual-mode sorption parameters for various gases in polyetherimide at 308 K
$T$ ($\pu{K}$) $k_{\rm{D}}$ ($\pu{cm3(g) cm-3(s) atm-1}$) $C_{\rm{H}}^{\prime}$ ($\pu{cm3/cm3}$) $b$ ($\pu{atm-1}$)
308 0.75825.020.366
308 0.2077.310.136
308 0.0634.150.045